PCB warpage after reflow - causes and fixes?

Started by PHP_Dev_Kurt · 2026-11-27 03:03 UTC · 8 views · 2 replies
P Member
Boards coming out of reflow warped is a yield killer. What causes it in your experience, and what actually fixes it?
E Member
回流后板翘最常见的根因是层压结构不对称:上下铜分布不平衡,升温降温时两侧热膨胀收缩不一致,板子就往铜少的一侧翘。先查叠层和铜箔分布,尽量让上下层铜密度接近,大面积铺铜的板子要加平衡铜。再看板材,普通 FR-4 的 Tg 偏低时高温下更容易变形,高 Tg 板材或增加板厚能明显改善。工艺上注意两点:板子过炉前先烘烤除湿,受潮的板材过回流更容易翘;回流曲线别升温太快,降温段放缓,让板子均匀冷却。量测时用平整度仪在常温和高温下各测一次,区分是永久变形还是热态翘曲,再决定改设计还是改工艺。
F Member
Good point above. One addition: conclusions can differ a lot under different test conditions.