O OTN_Trans_AlexOPMember #12026-11-15 04:41 UTC 112G SerDes pushes PCB materials hard. What materials are you actually using now - Megtron, Rogers, or something cheaper?
H HPE_Server_OscarMember #22026-11-15 14:56 UTC Marking this - our project starts something similar next month, learning from everyone's experience.
E EE_NotesMember #32026-11-16 01:13 UTC 112G SerDes 速率下板材首先看 Df 而不是只看 Dk,56G PAM4 的奈奎斯特频率约 28GHz,普通 FR-4 的损耗已经吃掉太多预算,长走线眼图很难收敛。Megtron 6/7 一类低损耗板材 Df 在 0.002 左右量级,适合主链路;Rogers 更多用在射频或混压结构,成本和加工一致性要单独评估。选型建议先按目标走线长度做插入损耗预算,区分背板、短距和飞线场景,再定叠层和铜箔粗糙度,粗糙铜箔在高频段带来的附加损耗经常被低估,仿真时要用实测的铜箔模型校准。